Skip to content
KORNDEX – Home

Sanding problem

Blisters in the paint over a filler repair

Also: Paint bubbles · Blisters over filler · Filler blistering

Why does the paint blister over the filler repair? Usually the filler was wet sanded. Polyester filler is porous, absorbs water and releases it under the paint. Filler should be dry sanded.

How to spot it

After painting, small blisters appear over a filled area – and nowhere else.

Where it comes from

  • The polyester filler was wet sanded: it is porous, soaks up the water and releases it later.
  • The primer surfacer was not fully cured when painted.
  • Fresh filler was sanded too early – soft material gums up and traps moisture.

What helps now

  • Always dry sand filler, with dust extraction – wet sanding is for the finished paint, not the substrate.
  • Primer surfacer may be wet sanded, but must then dry out completely.
  • Open up the area again, dry sand down to a sound base and build it up again.

Grits to put it right

Read the full sequence:Body filler Car & paint

In depth in the guides:Wet or dry sanding: which grit when? Sanding primer surfacer: wet or dry? What grit for sanding body filler?

More sanding defects